国标硬度计示值的最大允许误差
国标洛氏硬度计示值的最大允许误差
标尺 |
标准块的硬度范围 |
示值最大允许误差 |
HRA |
(20-75)HRA |
±2HRA |
(>75-88)HRA |
±1.5HRA |
|
HRB |
(20-45)HRB |
±4HRB |
(>45-80)HRB |
±3HRB |
|
(>80-100)HRB |
±2HRB |
|
HRC |
(20-70)HRC |
±1.5HRC |
HRD |
(40-70)HRD |
±2HRD |
(>70-77)HRD |
±1.5HRD |
|
HRE |
(70-90)HRE |
±2.5HRE |
(>90-100)HRE |
±2HRE |
|
HRF |
(60-90)HRF |
±3HRF |
(>90-100)HRF |
±2HRF |
|
HRG |
(30-50)HRG |
±6HRG |
(>50-75)HRG |
±4.5HRG |
|
(>75-94)HRG |
±3HRG |
|
HRH |
(80-100)HRH |
±2HRH |
HRK |
(40-60)HRK |
±4HRK |
(>60-80)HRK |
±3HRK |
|
(>80-100)HRK |
±2HRK |
|
HRL |
(100-120)HRL |
±1.2HRL |
HRM |
(85-110)HRM |
±1.5HRM |
HRR |
(114-125)HRR |
±1.2HRR |
国标维氏硬度计示值最大允许误差
硬度符号 |
硬度计示值的最大允许误差(±%) |
|||||||||||||||
硬度,HV |
||||||||||||||||
50 |
100 |
150 |
200 |
250 |
300 |
350 |
400 |
450 |
500 |
600 |
700 |
800 |
900 |
1000 |
||
HV0.05 |
6 |
8 |
9 |
10 |
|
|
|
|
|
|
|
|
|
|
|
|
HV0.1 |
5 |
6 |
7 |
8 |
8 |
9 |
10 |
10 |
11 |
|
|
|
|
|
|
|
HV0.2 |
|
4 |
|
6 |
|
8 |
|
9 |
|
10 |
11 |
11 |
12 |
12 |
|
|
HV0.3 |
|
4 |
|
5 |
|
6 |
|
7 |
|
8 |
9 |
10 |
10 |
11 |
11 |
|
HV0.5 |
|
3 |
|
5 |
|
5 |
|
6 |
|
6 |
7 |
7 |
8 |
8 |
9 |
|
HV1 |
|
3 |
|
4 |
|
4 |
|
4 |
|
5 |
5 |
5 |
6 |
6 |
6 |
|
HV2 |
|
3 |
|
3 |
|
3 |
|
4 |
|
4 |
4 |
4 |
4 |
5 |
5 |
|
HV3 |
|
3 |
|
3 |
|
3 |
|
3 |
|
3 |
4 |
4 |
4 |
4 |
4 |
|
HV5 |
|
3 |
|
3 |
|
3 |
|
3 |
|
3 |
3 |
3 |
3 |
3 |
4 |
|
HV10 |
|
3 |
|
3 |
|
3 |
|
3 |
|
3 |
3 |
3 |
3 |
3 |
3 |
|
HV20 |
|
3 |
|
3 |
|
3 |
|
3 |
|
3 |
3 |
3 |
3 |
3 |
3 |
|
HV30 |
|
3 |
|
3 |
|
2 |
|
2 |
|
2 |
2 |
2 |
2 |
2 |
2 |
|
HV50 |
|
3 |
|
3 |
|
2 |
|
2 |
|
2 |
2 |
2 |
2 |
2 |
2 |
|
HV100 |
|
|
|
3 |
|
2 |
|
2 |
|
2 |
2 |
2 |
2 |
2 |
2 |
|
注:
1.当压痕对角线长度小于 |
||||||||||||||||
国标布氏硬度计示值最大允许误差和示值重复性
硬度范围(HBW) |
示值最大允许误差δ% |
表示值重复性Hcf/% |
≦125 |
±3 |
≤3.5 |
125<HBW≤225 |
±2.5 |
≤3.0 |
>225 |
±2 |
≤2.5 |